<listing id="l9bhj"><var id="l9bhj"></var></listing>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<var id="l9bhj"></var><cite id="l9bhj"><video id="l9bhj"></video></cite>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"><listing id="l9bhj"></listing></strike></cite><cite id="l9bhj"><span id="l9bhj"><menuitem id="l9bhj"></menuitem></span></cite>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<ins id="l9bhj"><span id="l9bhj"></span></ins>
Volume 37 Issue 8
Jul.  2021
Turn off MathJax
Article Contents
GAO Meng, LIU Juan-hong, WU Ai-xiang. Corrosion and deterioration mechanism of water-rich filling materials in carbonate solutions[J]. Chinese Journal of Engineering, 2015, 37(8): 976-983. doi: 10.13374/j.issn2095-9389.2015.08.002
Citation: GAO Meng, LIU Juan-hong, WU Ai-xiang. Corrosion and deterioration mechanism of water-rich filling materials in carbonate solutions[J]. Chinese Journal of Engineering, 2015, 37(8): 976-983. doi: 10.13374/j.issn2095-9389.2015.08.002

Corrosion and deterioration mechanism of water-rich filling materials in carbonate solutions

doi: 10.13374/j.issn2095-9389.2015.08.002
  • Received Date: 2014-12-10
    Available Online: 2021-07-10
  • In order to research the impact of carbonate ions on water-rich filling materials,strength testing,scanning electron microscopy,X-ray diffraction analysis and IR spectrum testing were used to analyze the macro- and micro-structural change and the corrosion and deterioration mechanism of the materials in sodium carbonate solutions. It is found that the compressive strength of the materials in a sodium carbonate solution whose mass fraction is 10% decreases significantly with increasing soaking time. When the soak age is 90 d,the compressive strength of the materials decreases by 72.5% compared with standard curing for 28 d. After soaking for 28 d the specimen surface is muddy. XRD patterns show that after soaking in a sodium carbonate solution whose mass fraction is 10%,thaumasite generates in the materials. With increasing soaking time the amount of thaumasite increases. Infrared spectroscopy results show that there does not exist[AlO6]. This confirms that ettringite in the materials soaking in the sodium carbonate solution drastically reduces and transforms into pulpy thaumasite. As non-cemented materials,thaumasite will cause serious damage to the hardening body of the materials. This shows that the carbonate solution has corrosive action on water-rich filling materials.

     

  • loading
  • 加載中

Catalog

    通訊作者: 陳斌, bchen63@163.com
    • 1. 

      沈陽化工大學材料科學與工程學院 沈陽 110142

    1. 本站搜索
    2. 百度學術搜索
    3. 萬方數據庫搜索
    4. CNKI搜索
    Article views (434) PDF downloads(10) Cited by()
    Proportional views
    Related

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return
    久色视频