<listing id="l9bhj"><var id="l9bhj"></var></listing>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<var id="l9bhj"></var><cite id="l9bhj"><video id="l9bhj"></video></cite>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"><listing id="l9bhj"></listing></strike></cite><cite id="l9bhj"><span id="l9bhj"><menuitem id="l9bhj"></menuitem></span></cite>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<ins id="l9bhj"><span id="l9bhj"></span></ins>
Volume 37 Issue 5
Jul.  2021
Turn off MathJax
Article Contents
DING Xian-fei, CHEN Xue-da, LI Qing, XIAO Cheng-bo, REN Wei-peng, FENG Qiang. Salt-deposit hot corrosion behaviors of directionally solidified DZ466 superalloy[J]. Chinese Journal of Engineering, 2015, 37(5): 608-614. doi: 10.13374/j.issn2095-9389.2015.05.011
Citation: DING Xian-fei, CHEN Xue-da, LI Qing, XIAO Cheng-bo, REN Wei-peng, FENG Qiang. Salt-deposit hot corrosion behaviors of directionally solidified DZ466 superalloy[J]. Chinese Journal of Engineering, 2015, 37(5): 608-614. doi: 10.13374/j.issn2095-9389.2015.05.011

Salt-deposit hot corrosion behaviors of directionally solidified DZ466 superalloy

doi: 10.13374/j.issn2095-9389.2015.05.011
  • Received Date: 2015-03-03
    Available Online: 2021-07-10
  • Hot corrosion behaviors of DZ466 alloy at 850℃ and 950℃ were investigated by using a NaCl/Na2SO4salt-deposit method. It is found that there are three corrosion layers on the alloy. The outer and the middle layers consist of(Ni,Co) O oxide and(Ni,Co) Cr2O4 with a spinel structure,respectively. The innermost layer is an inner corrosion layer,which consists of Ni3S2 at 850℃,and the internal oxidation Al2O3 can be produced close to the middle layer at 950℃. The same hot corrosion mechanism is shown at 850℃ and 950℃. The destruction of the oxidation film continuity is a key reason for hot corrosion of the alloy. The hot corrosion weight gain curves obey a parabolic law at the two temperatures,the rate constants are 3.1×10-11g2·cm-4·s-1 and 1.5 × 10-9g2·cm-4·s-1,and the hot corrosion activation energies are 179.2 and 138.3 kJ ·mol-1at 850℃ and 950℃,respectively.

     

  • loading
  • 加載中

Catalog

    通訊作者: 陳斌, bchen63@163.com
    • 1. 

      沈陽化工大學材料科學與工程學院 沈陽 110142