<listing id="l9bhj"><var id="l9bhj"></var></listing>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<var id="l9bhj"></var><cite id="l9bhj"><video id="l9bhj"></video></cite>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"><listing id="l9bhj"></listing></strike></cite><cite id="l9bhj"><span id="l9bhj"><menuitem id="l9bhj"></menuitem></span></cite>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<ins id="l9bhj"><span id="l9bhj"></span></ins>
Volume 35 Issue 5
Jul.  2021
Turn off MathJax
Article Contents
ZHU Hong-wu, LIU Ya-zheng, ZHOU Le-yu, WANG Lei-ying, HUANG Bin. Failure analysis of 22Si2MnCrNi2MoA drilling rods[J]. Chinese Journal of Engineering, 2013, 35(5): 613-619. doi: 10.13374/j.issn1001-053x.2013.05.009
Citation: ZHU Hong-wu, LIU Ya-zheng, ZHOU Le-yu, WANG Lei-ying, HUANG Bin. Failure analysis of 22Si2MnCrNi2MoA drilling rods[J]. Chinese Journal of Engineering, 2013, 35(5): 613-619. doi: 10.13374/j.issn1001-053x.2013.05.009

Failure analysis of 22Si2MnCrNi2MoA drilling rods

doi: 10.13374/j.issn1001-053x.2013.05.009
  • Received Date: 2011-12-04
  • The fracture of a 22Si2MnCrNi2MoA drilling rod near the internal thread was analyzed in term of the microstructure, inclusions and fractograph by means of optical microscopy, scanning electron microscopy and energy dispersive spectroscopy. Fatigue crack initiation and propagation in the drilling rod were studied. It is found that the fracture of the drilling rod is not induced by the abnormal microstructure and inclusions. Instead, because the wall thickness of the drilling rod near the internal thread is obviously uneven, the area with a thinner wall thickness tends to be the weak load-bearing point under the continuous stress of high frequency, serious outside consumption and internal friction existing simultaneously. Thus fatigue cracks are likely to emerge in the area preferentially. After that, the drilling rod ruptures in the area and eventually fractures. Furthermore, this fatigue failure is originated from the inside surface of the drilling rod and it belongs to the fatigue fracture with many crack sources. The morphology of the zones around the crack sources is dimple fracture, but the morphology of the zones of crack propagation is a mixed type with dimple and intergranular fracture.

     

  • loading
  • 加載中

Catalog

    通訊作者: 陳斌, bchen63@163.com
    • 1. 

      沈陽化工大學材料科學與工程學院 沈陽 110142

    1. 本站搜索
    2. 百度學術搜索
    3. 萬方數據庫搜索
    4. CNKI搜索
    Article views (261) PDF downloads(7) Cited by()
    Proportional views
    Related

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return
    久色视频