<listing id="l9bhj"><var id="l9bhj"></var></listing>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<var id="l9bhj"></var><cite id="l9bhj"><video id="l9bhj"></video></cite>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"><listing id="l9bhj"></listing></strike></cite><cite id="l9bhj"><span id="l9bhj"><menuitem id="l9bhj"></menuitem></span></cite>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<ins id="l9bhj"><span id="l9bhj"></span></ins>
Volume 34 Issue 4
Jul.  2021
Turn off MathJax
Article Contents
LIU Ji-xiong, ZHAO Ai-min, JIANG Hai-tao, TANG Di, SHUI Heng-yong. In-situ SEM observation on titanium clad steel plates in the bending process[J]. Chinese Journal of Engineering, 2012, 34(4): 424-429. doi: 10.13374/j.issn1001-053x.2012.04.007
Citation: LIU Ji-xiong, ZHAO Ai-min, JIANG Hai-tao, TANG Di, SHUI Heng-yong. In-situ SEM observation on titanium clad steel plates in the bending process[J]. Chinese Journal of Engineering, 2012, 34(4): 424-429. doi: 10.13374/j.issn1001-053x.2012.04.007

In-situ SEM observation on titanium clad steel plates in the bending process

doi: 10.13374/j.issn1001-053x.2012.04.007
  • Received Date: 2011-02-09
    Available Online: 2021-07-30
  • Two titanium clad steel plates were prepared by exploding and exploding-rolling,respectively.In order to study the fracture behavior of the clad plates during the bending process,crack initiation and propagation were observed by scanning electron microscopy(SEM).The result shows that the crack initiation angle in external bending is less than that in internal bending,the capability of resistance to crack initiation in internal bending is stronger than that in external bending,but.During the bending process,cracks in the exploding clad plate mainly initiate on the interface junction of wave front and the center of whirlpools,but cracks in the exploding-rolling clad plate initiate at the hard lump interfaces of Ti-Fe intermetallic compounds.The main reason of cracking is that the interface junction of wave front and the center of whirlpools of the exploding titanium clad steel plate and Ti-Fe intermetallic compounds in the exploding-and-rolling clad plate are difficult to compatibly deform because of their high hardness.

     

  • loading
  • 加載中

Catalog

    通訊作者: 陳斌, bchen63@163.com
    • 1. 

      沈陽化工大學材料科學與工程學院 沈陽 110142

    1. 本站搜索
    2. 百度學術搜索
    3. 萬方數據庫搜索
    4. CNKI搜索
    Article views (294) PDF downloads(8) Cited by()
    Proportional views
    Related

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return
    久色视频