<listing id="l9bhj"><var id="l9bhj"></var></listing>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<var id="l9bhj"></var><cite id="l9bhj"><video id="l9bhj"></video></cite>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"><listing id="l9bhj"></listing></strike></cite><cite id="l9bhj"><span id="l9bhj"><menuitem id="l9bhj"></menuitem></span></cite>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<ins id="l9bhj"><span id="l9bhj"></span></ins>
Volume 32 Issue 9
Aug.  2021
Turn off MathJax
Article Contents
CENG Li, REN Xue-ping, LU Shang-wen, CUI Yan. High-temperature backward extrusion forming of aluminum matrix composite cup-shaped parts with high volume fraction of SiCp[J]. Chinese Journal of Engineering, 2010, 32(9): 1186-1191. doi: 10.13374/j.issn1001-053x.2010.09.011
Citation: CENG Li, REN Xue-ping, LU Shang-wen, CUI Yan. High-temperature backward extrusion forming of aluminum matrix composite cup-shaped parts with high volume fraction of SiCp[J]. Chinese Journal of Engineering, 2010, 32(9): 1186-1191. doi: 10.13374/j.issn1001-053x.2010.09.011

High-temperature backward extrusion forming of aluminum matrix composite cup-shaped parts with high volume fraction of SiCp

doi: 10.13374/j.issn1001-053x.2010.09.011
  • Received Date: 2009-12-08
  • An aluminum matrix composite with high volume fraction of SiCp was prepared by pressureless infiltration.Cup-shaped parts were made of the SiCp/Al composite by using high temperature backward extrusion.The flow stress behavior of the SiCp/Al composite during hot backward extrusion was investigated.The effects of hot backward extrusion parameters on the microstructure of the SiCp/Al composite were observed and analyzed by SEM.The results show that at temperatures above the melting point of aluminum matrix the SiCp/Al composite is a viscous fluid,SiC particles and aluminum matrix form into a solid-liquid mixture.When the SiCp/Al composite is backward extruded at high temperature,aluminum matrix remains continuous,but SiC particles roll over and rearrange under pressure,some particles break,and the particle distribution uniformity is good.As the deformation temperature is lower and the extrusion speed is rapider,SiC particles are easy to break,the internal particle size distribution of SiCp/Al composite cup-shaped parts is nonuniform,and the particle size is smaller in the internal angle position of cup-shaped parts.The particle size uniformly distributes at a higher temperature and a smaller extrusion speed.

     

  • loading
  • 加載中

Catalog

    通訊作者: 陳斌, bchen63@163.com
    • 1. 

      沈陽化工大學材料科學與工程學院 沈陽 110142

    1. 本站搜索
    2. 百度學術搜索
    3. 萬方數據庫搜索
    4. CNKI搜索
    Article views (176) PDF downloads(6) Cited by()
    Proportional views
    Related

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return
    久色视频