<listing id="l9bhj"><var id="l9bhj"></var></listing>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<var id="l9bhj"></var><cite id="l9bhj"><video id="l9bhj"></video></cite>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"><listing id="l9bhj"></listing></strike></cite><cite id="l9bhj"><span id="l9bhj"><menuitem id="l9bhj"></menuitem></span></cite>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<ins id="l9bhj"><span id="l9bhj"></span></ins>
Volume 26 Issue 6
Aug.  2021
Turn off MathJax
Article Contents
ZHENG Hongguang, CHEN Weiqing, LI Zhien, LI Xuefeng. Different Mechanisms of Clogging in Continuous Casting of Type 304 and 321 Stainless Steels[J]. Chinese Journal of Engineering, 2004, 26(6): 596-599. doi: 10.13374/j.issn1001-053x.2004.06.033
Citation: ZHENG Hongguang, CHEN Weiqing, LI Zhien, LI Xuefeng. Different Mechanisms of Clogging in Continuous Casting of Type 304 and 321 Stainless Steels[J]. Chinese Journal of Engineering, 2004, 26(6): 596-599. doi: 10.13374/j.issn1001-053x.2004.06.033

Different Mechanisms of Clogging in Continuous Casting of Type 304 and 321 Stainless Steels

doi: 10.13374/j.issn1001-053x.2004.06.033
  • Received Date: 2004-01-14
    Available Online: 2021-08-17
  • The clogs on the submerged entry nozzle of type 304 and 321 stainless steels were investigated, and the mechanisms of clogging were discussed. The results indicated that deposits on the nozzle in type 304 stainless steel consists of Al2O3, MgO·Al2O3 and some metal. Because of the thin deposits, the casting was not affected obviously and could be improved by controlling [Al] < 0.01 %. There are two kinds of clogging, namely TiN-type and CaO·TiO2-type clogging, in the casting of type 321 stainless steel. TiN-type clogging consists of a lot of TiN inclusions and some metal, and could be improved by [Ti%]·[N%]×103 < 3.5 and [Al] < 0.01% in liquid. CaO·TiO2 type clogging consists of CaO-TiO2-MgO-Al2O3 and a lot of metal, and could be improved obviously by reducing the amount of CaO-TiO2-MgO-Al2O3 inclusions in molten steel.

     

  • loading
  • 加載中

Catalog

    通訊作者: 陳斌, bchen63@163.com
    • 1. 

      沈陽化工大學材料科學與工程學院 沈陽 110142

    1. 本站搜索
    2. 百度學術搜索
    3. 萬方數據庫搜索
    4. CNKI搜索
    Article views (236) PDF downloads(12) Cited by()
    Proportional views
    Related

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return
    久色视频