<listing id="l9bhj"><var id="l9bhj"></var></listing>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<var id="l9bhj"></var><cite id="l9bhj"><video id="l9bhj"></video></cite>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"><listing id="l9bhj"></listing></strike></cite><cite id="l9bhj"><span id="l9bhj"><menuitem id="l9bhj"></menuitem></span></cite>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<ins id="l9bhj"><span id="l9bhj"></span></ins>
Volume 25 Issue 5
Aug.  2021
Turn off MathJax
Article Contents
WANG Hongbin, CHEN Meiying, LIU Huimin, HUANG Jinfeng, YANG Bin, ZHANG Jishan. Experimental Investigation on Heat Treatment of Spray-Forming Ultrahigh Strength Al-Zn-Mg-Cu Alloys[J]. Chinese Journal of Engineering, 2003, 25(5): 436-440. doi: 10.13374/j.issn1001-053x.2003.05.039
Citation: WANG Hongbin, CHEN Meiying, LIU Huimin, HUANG Jinfeng, YANG Bin, ZHANG Jishan. Experimental Investigation on Heat Treatment of Spray-Forming Ultrahigh Strength Al-Zn-Mg-Cu Alloys[J]. Chinese Journal of Engineering, 2003, 25(5): 436-440. doi: 10.13374/j.issn1001-053x.2003.05.039

Experimental Investigation on Heat Treatment of Spray-Forming Ultrahigh Strength Al-Zn-Mg-Cu Alloys

doi: 10.13374/j.issn1001-053x.2003.05.039
  • Received Date: 2002-01-05
    Available Online: 2021-08-17
  • The microstructures of as-deposited and extruded ultrahigh strength aluminum alloys by spray-forming were investigated. The aging-curves and tensile properties were tested after solid-solution treatment and aging treatment. The result shows that in as-deposited alloys, many porosities are obvious. In extruded alloys, however, there are large amount of Cu-rich particles. The solid-solution treatment temperature should not be higher than 490℃ because much of grain-boundaries melt in this temperature. At 120℃, the time to obtain hardness peaks ranges from 15 to 25 h. At 135℃, the relationship is obvious between the time and the composition of the alloys:The more Zn contented, the less the time; the tensile strength of the alloys keeps on about 700 MPa.

     

  • loading
  • 加載中

Catalog

    通訊作者: 陳斌, bchen63@163.com
    • 1. 

      沈陽化工大學材料科學與工程學院 沈陽 110142

    1. 本站搜索
    2. 百度學術搜索
    3. 萬方數據庫搜索
    4. CNKI搜索
    Article views (166) PDF downloads(11) Cited by()
    Proportional views
    Related

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return
    久色视频