<listing id="l9bhj"><var id="l9bhj"></var></listing>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<var id="l9bhj"></var><cite id="l9bhj"><video id="l9bhj"></video></cite>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"><listing id="l9bhj"></listing></strike></cite><cite id="l9bhj"><span id="l9bhj"><menuitem id="l9bhj"></menuitem></span></cite>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<ins id="l9bhj"><span id="l9bhj"></span></ins>
Volume 34 Issue 7
Jul.  2021
Turn off MathJax
Article Contents
JIANG Hai-tao, LU Chun-jie, DUAN Xiao-ge, TANG Di, LI Zhi-chao. Hot deformation processing map of AZ31 magnesium alloy and its application[J]. Chinese Journal of Engineering, 2012, 34(7): 808-812. doi: 10.13374/j.issn1001-053x.2012.07.013
Citation: JIANG Hai-tao, LU Chun-jie, DUAN Xiao-ge, TANG Di, LI Zhi-chao. Hot deformation processing map of AZ31 magnesium alloy and its application[J]. Chinese Journal of Engineering, 2012, 34(7): 808-812. doi: 10.13374/j.issn1001-053x.2012.07.013

Hot deformation processing map of AZ31 magnesium alloy and its application

doi: 10.13374/j.issn1001-053x.2012.07.013
  • Received Date: 2011-05-24
    Available Online: 2021-07-30
  • To determine the deformation parameters of AZ31 magnesium alloy, the hot deformation behavior of the alloy was investigated by hot compression testing on a Gleeble-3500 stimulator. The principle of dynamic material modeling was used to develop the hot processing map. There is a dynamic recrystallization peak zone in the processing map at temperatures from 380 to 400℃ and strain rates from 3 to 12 s-1, and the efficiency of power dissipation is more than 30%. A fine equiaxed grain size of 2.3 μm could be achieved when differential speed rolling is processed in this region. The tensile strength is 322.7 MPa and the elongation is 19.6%. At strain rates of 15 to 50 s-1, there are two flow instability zones:at temperatures of 250 to 300℃ the ductility of the alloy decreases obviously, but at temperatures of 350 to 400℃ the alloy has a mischcrystal structure.

     

  • loading
  • 加載中

Catalog

    通訊作者: 陳斌, bchen63@163.com
    • 1. 

      沈陽化工大學材料科學與工程學院 沈陽 110142

    1. 本站搜索
    2. 百度學術搜索
    3. 萬方數據庫搜索
    4. CNKI搜索
    Article views (182) PDF downloads(11) Cited by()
    Proportional views
    Related

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return
    久色视频