<listing id="l9bhj"><var id="l9bhj"></var></listing>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<var id="l9bhj"></var><cite id="l9bhj"><video id="l9bhj"></video></cite>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"><listing id="l9bhj"></listing></strike></cite><cite id="l9bhj"><span id="l9bhj"><menuitem id="l9bhj"></menuitem></span></cite>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<ins id="l9bhj"><span id="l9bhj"></span></ins>
Volume 34 Issue 7
Jul.  2021
Turn off MathJax
Article Contents
NIE Jun-hui, ZHANG Ya-feng, SHI Na, JIA Cheng-chang. Fabrication and properties of Cu matrix composites reinforced by tungsten-coated carbon nanotubes[J]. Chinese Journal of Engineering, 2012, 34(7): 823-829. doi: 10.13374/j.issn1001-053x.2012.07.004
Citation: NIE Jun-hui, ZHANG Ya-feng, SHI Na, JIA Cheng-chang. Fabrication and properties of Cu matrix composites reinforced by tungsten-coated carbon nanotubes[J]. Chinese Journal of Engineering, 2012, 34(7): 823-829. doi: 10.13374/j.issn1001-053x.2012.07.004

Fabrication and properties of Cu matrix composites reinforced by tungsten-coated carbon nanotubes

doi: 10.13374/j.issn1001-053x.2012.07.004
  • Received Date: 2011-05-16
    Available Online: 2021-07-30
  • Multi-walled carbon nanotubes (CNTs) were coated with tungsten layers using a carbonyl thermal decomposition process. The tungsten-coated carbon nanotubes (W-CNTs) and electrolytic copper powders were used as starting materials to fabricated W-CNT/Cu composites by mechanical milling and spark plasma sintering (SPS). The morphologies and microstructures of the mixed powders and the sintered composite bulks were characterized by field-emission scanning electron microscopy (SEM), and the phase analysis of the sintered composite bulks was carried out by X-ray diffraction (XRD). The influences of W-CNT content and sintering temperature on the relative density, tensile strength, elongation and electrical conductivity of the W-CNT/Cu composites were investigated. The experimental results show that the 1% W-CNT added composites sintered at 850℃ have the maximum relative density, tensile strength and electrical conductivity. In comparison with the sintered pure Cu bulk, the tensile strength increases by 103.6% but the electrical conductivity decreases only by 15.9% for the W-CNT/Cu composites.

     

  • loading
  • 加載中

Catalog

    通訊作者: 陳斌, bchen63@163.com
    • 1. 

      沈陽化工大學材料科學與工程學院 沈陽 110142

    1. 本站搜索
    2. 百度學術搜索
    3. 萬方數據庫搜索
    4. CNKI搜索
    Article views (335) PDF downloads(8) Cited by()
    Proportional views
    Related

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return
    久色视频