<listing id="l9bhj"><var id="l9bhj"></var></listing>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<var id="l9bhj"></var><cite id="l9bhj"><video id="l9bhj"></video></cite>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"><listing id="l9bhj"></listing></strike></cite><cite id="l9bhj"><span id="l9bhj"><menuitem id="l9bhj"></menuitem></span></cite>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<ins id="l9bhj"><span id="l9bhj"></span></ins>
Volume 33 Issue 12
Jul.  2021
Turn off MathJax
Article Contents
XU Li-ning, TAN Hui-min, CHANG Wei, ZHANG Lei, LU Min-xu, LI Shao-fei. CO2 corrosion behavior of X70 pipeline steel in wet gas environment[J]. Chinese Journal of Engineering, 2011, 33(12): 1478-1484. doi: 10.13374/j.issn1001-053x.2011.12.009
Citation: XU Li-ning, TAN Hui-min, CHANG Wei, ZHANG Lei, LU Min-xu, LI Shao-fei. CO2 corrosion behavior of X70 pipeline steel in wet gas environment[J]. Chinese Journal of Engineering, 2011, 33(12): 1478-1484. doi: 10.13374/j.issn1001-053x.2011.12.009

CO2 corrosion behavior of X70 pipeline steel in wet gas environment

doi: 10.13374/j.issn1001-053x.2011.12.009
  • Received Date: 2010-12-22
    Available Online: 2021-07-30
  • With a high-temperature and high-pressure condensation autoclave simulating the circumstance of CO2 corrosion in wet gas pipelines,the variation in corrosion behavior and morphology of X70 pipeline steel was studied by changing the wet gas temperature and the temperature difference between the wet gas and the pipe wall.Scanning electron microscopy(SEM) and energy dispersive spectrometry(EDS) were employed to analyze the morphologies and characteristics of corrosion scales on the steel.The results were compared with those under solution-immersed conditions in a high-temperature and high-pressure autoclave.Using a corrosion prediction model,the influence of some important parameters on corrosion at the top of wet gas pipelines were preliminary studied,such as wet gas and pipe wall temperatures,temperature difference,condensed liquid film temperature and condensation rate.The results show that at the same temperature of the pipe wall(5℃),the corrosion rate increases with the wet gas temperature rising;while at the same temperature of wet gas(25℃ and 45℃),the corrosion rate decreases slightly with the pipe wall temperature rising.In the temperature range of 20 to 45℃,corrosion scales are easily peeled off from the substrate,and uniform corrosion is the predominant morphology.

     

  • loading
  • 加載中

Catalog

    通訊作者: 陳斌, bchen63@163.com
    • 1. 

      沈陽化工大學材料科學與工程學院 沈陽 110142

    1. 本站搜索
    2. 百度學術搜索
    3. 萬方數據庫搜索
    4. CNKI搜索
    Article views (304) PDF downloads(7) Cited by()
    Proportional views
    Related

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return
    久色视频