<listing id="l9bhj"><var id="l9bhj"></var></listing>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<var id="l9bhj"></var><cite id="l9bhj"><video id="l9bhj"></video></cite>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"><listing id="l9bhj"></listing></strike></cite><cite id="l9bhj"><span id="l9bhj"><menuitem id="l9bhj"></menuitem></span></cite>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<ins id="l9bhj"><span id="l9bhj"></span></ins>
Volume 33 Issue 11
Jul.  2021
Turn off MathJax
Article Contents
TIAN Chang-juan, HE Xin-bo, MEI Min, QU Xuan-hui. Si3N4 particle-reinforced 316L stainless steel prepared by powder injection molding[J]. Chinese Journal of Engineering, 2011, 33(11): 1373-1377. doi: 10.13374/j.issn1001-053x.2011.11.020
Citation: TIAN Chang-juan, HE Xin-bo, MEI Min, QU Xuan-hui. Si3N4 particle-reinforced 316L stainless steel prepared by powder injection molding[J]. Chinese Journal of Engineering, 2011, 33(11): 1373-1377. doi: 10.13374/j.issn1001-053x.2011.11.020

Si3N4 particle-reinforced 316L stainless steel prepared by powder injection molding

doi: 10.13374/j.issn1001-053x.2011.11.020
  • Received Date: 2010-12-02
    Available Online: 2021-07-30
  • Si3N4 particle-reinforced 316L stainless steel composites were prepared by powder injection molding(PIM) using water-soluble binders.It is shown that a water-soluble binder mainly consisting of polyoxymethylene(PEG),polyvinyl butyral(PVB) and stearic acid(SA) exhibits a better water-soluble degreasing performance.After degreasing injection parts in water for 6 h,the total binder removal rate is 55% and the PEG removal rate is 78.6%.The sintered composites have a uniform microstructure and excellent properties with a relative density of 95.2%,a hardness of HRB 79.8 and a tensile strength of 620 MPa.And the hardness and tensile strength are 5% and 20.4% higher than the Si3N4 particle-reinforced 316L stainless steel produced by PIM with a paraffin wax-based binder,respectively.

     

  • loading
  • 加載中

Catalog

    通訊作者: 陳斌, bchen63@163.com
    • 1. 

      沈陽化工大學材料科學與工程學院 沈陽 110142

    1. 本站搜索
    2. 百度學術搜索
    3. 萬方數據庫搜索
    4. CNKI搜索
    Article views (155) PDF downloads(7) Cited by()
    Proportional views
    Related

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return
    久色视频