<listing id="l9bhj"><var id="l9bhj"></var></listing>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<var id="l9bhj"></var><cite id="l9bhj"><video id="l9bhj"></video></cite>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"><listing id="l9bhj"></listing></strike></cite><cite id="l9bhj"><span id="l9bhj"><menuitem id="l9bhj"></menuitem></span></cite>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<ins id="l9bhj"><span id="l9bhj"></span></ins>
Volume 33 Issue 3
Jul.  2021
Turn off MathJax
Article Contents
LI Ju-yan, WEN Guang-hua, TANG Ping, LI Jian-quan, XIANG Cheng-li. Analysis on corner transverse cracks of slabs with different section dimensions cast with Pangang slab casting machine[J]. Chinese Journal of Engineering, 2011, 33(3): 296-301. doi: 10.13374/j.issn1001-053x.2011.03.015
Citation: LI Ju-yan, WEN Guang-hua, TANG Ping, LI Jian-quan, XIANG Cheng-li. Analysis on corner transverse cracks of slabs with different section dimensions cast with Pangang slab casting machine[J]. Chinese Journal of Engineering, 2011, 33(3): 296-301. doi: 10.13374/j.issn1001-053x.2011.03.015

Analysis on corner transverse cracks of slabs with different section dimensions cast with Pangang slab casting machine

doi: 10.13374/j.issn1001-053x.2011.03.015
  • Received Date: 2010-06-01
    Available Online: 2021-07-30
  • The effect of cooling conditions on the corner transverse cracks of slabs with different section dimensions was studied by nozzle performance measurements, remehing and solidification cooling experiments and numerical simulations. The results show that the corner temperature is lower than the A3 temperature earlier for slabs with section dimensions of 1000, 1160 and 1250 mm during a stronger cooling. There is a large number of film-like proeutectoid ferrite along grain boundaries, and transverse cracks form along prior austenite grain boundaries when straightening. To prevent from these transverse cracks, a process to control the surfaee mierostrueture of a slab was adopted and applied to actual production at Pansteel.

     

  • loading
  • 加載中

Catalog

    通訊作者: 陳斌, bchen63@163.com
    • 1. 

      沈陽化工大學材料科學與工程學院 沈陽 110142

    1. 本站搜索
    2. 百度學術搜索
    3. 萬方數據庫搜索
    4. CNKI搜索
    Article views (161) PDF downloads(11) Cited by()
    Proportional views
    Related

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return
    久色视频