<listing id="l9bhj"><var id="l9bhj"></var></listing>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<cite id="l9bhj"><strike id="l9bhj"></strike></cite>
<var id="l9bhj"></var><cite id="l9bhj"><video id="l9bhj"></video></cite>
<menuitem id="l9bhj"></menuitem>
<cite id="l9bhj"><strike id="l9bhj"><listing id="l9bhj"></listing></strike></cite><cite id="l9bhj"><span id="l9bhj"><menuitem id="l9bhj"></menuitem></span></cite>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"></var>
<var id="l9bhj"><strike id="l9bhj"></strike></var>
<ins id="l9bhj"><span id="l9bhj"></span></ins>
Volume 9 Issue 2
Oct.  2021
Turn off MathJax
Article Contents
Karpiliansky N. N., Li Hong, Wang Youming, Lu Shouli. Investigation of Superplasticity in Powder White Cast Iron Alloy[J]. Chinese Journal of Engineering, 1987, 9(2): 40-47. doi: 10.13374/j.issn1001-053x.1987.02.006
Citation: Karpiliansky N. N., Li Hong, Wang Youming, Lu Shouli. Investigation of Superplasticity in Powder White Cast Iron Alloy[J]. Chinese Journal of Engineering, 1987, 9(2): 40-47. doi: 10.13374/j.issn1001-053x.1987.02.006

Investigation of Superplasticity in Powder White Cast Iron Alloy

doi: 10.13374/j.issn1001-053x.1987.02.006
  • Received Date: 1986-07-14
    Available Online: 2021-10-28
  • White cast iron powder containing 2.875 Pct. C, l.3pct Cr was obtained by rapid solidification technology. The fully densified compact mat erial for testing has been prepared by the warm isostatic pressing (WIP) method at 720℃ for three hours with pressure of 150 MPa. The structure consisting of 1 to 3 μm in size ferrite grains and Cementite part-ides smaller than 3.5 in size was developed after WIP-uPsetting at 63 pct. strain. Superplastic behavior of the materials after WIP and WIP + upsetting were investigated in the temperature range 670-770℃ at strain rates from 3×10-4 to 1 s-1. At low stresses, the superplastic white cast iron exhibited a high strain rate sensitivity exponentm of 0.42 attemperature 720℃ arid ε=3.10-3~3.10-2S-1, it could develop a new proc eessing routes for new industrial applications.

     

  • loading
  • 加載中

Catalog

    通訊作者: 陳斌, bchen63@163.com
    • 1. 

      沈陽化工大學材料科學與工程學院 沈陽 110142

    1. 本站搜索
    2. 百度學術搜索
    3. 萬方數據庫搜索
    4. CNKI搜索
    Article views (248) PDF downloads(8) Cited by()
    Proportional views
    Related

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return
    久色视频